Lecture 5 & 6

Manual Metal Arc Welding:

Manual metal arc welding (MMAW) or shielded metal arc welding (SMAW) is the oldest and most widely used process being used for fabrication. The arc is struck between a flux covered stick electrode and the workpieces. The workpieces are made part of an electric circuit, known as welding circuit. It includes welding power source, welding cables, electrode holder, earth clamp and the consumable coated electrode. Figure 5.1 Shows details of welding circuit.

Fig 5.1: Manual Metal Arc Welding Circuit

Fig 5.2: Molten Metal and Flux Transfer to Weld Pool

Figure 5.2 shows the fine molten droplets of metal and molten flux coming from the tip of the coated electrode. The flux melts along with the metallic core wire and goes to weld pool where it reacts with molten metal forming slag which floats on the top of molten weld pool and solidifies after solidification of molten metal and can be removed by chipping and brushing.

Welding power sources used may be transformer or rectifier for AC or DC supply. The requirement depends on the type of electrode coating and sometimes on the material to be welded.

The constant-current or drooping type of power source is preferred for manual metal arc welding since it is difficult to hold a constant arc length. The changing arc length causes arc voltage to increase or decrease, which in turn produces a change in welding current. The steeper the slope of the volt-ampere curve within the welding range, the smaller the current change for a given change in arc voltage. This results into stable arc, uniform penetration and better weld seam inspite of fluctuations of arc length.

The welding voltages range from 20 to 30 V depending upon welding current i.e. higher the current, higher the voltage. Welding current depends on the size of the electrode i.e. core diameter. The approximate average welding current for structural steel electrodes is 35.d (where d is electrode diameter in mm) with some variations with the type of coating of electrode. Table 5.1 shows influence of welding parameters on weld characteristics.

Table 5.1: Welding Variables and Their Influence

Welding Condition

Main Effects

Current in excess of optimum

Excess spatter. Flat wide deposit. Deep crater. Deep penetration. Electrode overheats.

Current less than optimum

Slag difficult to control. Metal piles up. Poor dead shape. Poor penetration.

Voltage in excess of optimum

Deposit irregular and flat. Arc wander. Porosity. Spatter.

Voltage less than optimum

Irregular piling of weld metal. Arc extinctions. Little penetration.

Travel speed in excess of optimum

Narrow thin weld bead. Undercut.

Travel speed less than optimum

Wide thick deposit. Difficulty in slag control.

Optimum Welding conditions

Smooth even weld deposit. Stable arc condition. Easily controlled slag. Little spatter produced.

The output voltage of the power source on ‘no load' or ‘open circuit' must be high enough to enable the arc to be started. A value of 80 V is sufficient for most electrodes but certain types may require more or less than this value.

A manual welding power source is never loaded continuously because of operations such as, electrode changing, slag removal etc. Most MMA welding equipment has a duty cycle of around 40% at maximum welding current.

Coated Electrodes are specified based on core wire diameter. Commonly used electrode diameters are 2, 2.5, 3.18, 4, 5 and 6 mm. Length of electrodes may depend on diameter of core wire ranging from 250 to 450 mm i.e. larger the core diameter larger the length. However, special electrodes may be of 8-10 mm diameter. Table 5.2 gives the details of electrode sizes and currents.

Table 5.2: Size and Welding Current for Stick Mild Steel Electrodes

Diameter d mm

2.0

2.5

3.18(1/8")

4.0

5.0

6.0

Length L mm

250/300

350

350/450

450

450

450

Welding I Current A

50-80

70-100

90-130

120-160

160-200

190-240

The electrodes are also specified based on ratio of diameter of coated portion of electrode to core wire diameter. If this ratio is lesser than 1.2 then electrodes are thin coated, if ratio ranges between 1.2 to 1.5 then medium coated and if ratio exceeds 1.5 then electrodes are heavy coated or thick coated. This ratio may vary slightly in different codes.

Thin coated electrodes have very good bridgeability at the joint gap but weld bead has coarse ripples and penetration is also poor. Medium coated electrodes lead to reasonably good bridgeability, medium ripples in weld bead and modest penetration. Thick coated electrodes have poor bridgeability, however, bead appearance is excellent with fine ripples and also excellent penetration.

The ingress of oxygen and nitrogen from the atmosphere to the weld pool and arc environment would cause embrittlement and porosity in the weld metal and this must be prevented. The Actual method of arc shielding from atmospheric nitrogen and oxygen attack varies with different type of electrodes which are in two main categories.

1. Bulk of covering material converts to a gas by the heat of the arc, only a small amount of slag is produced. Protection depends largely upon a gaseous shield to prevent atmospheric contamination as in case of cellulosic electrode.

2. Bulk of covering material converts to a slag, only a small volume of shielding gas produced as in the case of rutile and basic coated electrodes.

Electrode coating performs many functions depending upon coating constituents, during welding to improve weld metal properties. The important functions are as follows:

1. Improve the electric conductivity in the arc region to improve the arc ignition and stabilization of the arc.

2. Formation of slag, which;

(a) Influences size of droplet.

(b) Protects the droplet during transfer and molten weld pool from atmospheric gases.

(c) Protects solidified hot metal from atmospheric gases.

(d) Reduces the cooling rate of weld seam.

3. Formation of shielding gas to protect molten metal.

4. Provide deoxidizers like Si and Mn in form of FeSi and FeMn.

5. Alloying with certain elements such as Cr, Ni, Mo to improve weld metal properties.

6. Improve deposition rate with addition of iron powder in coating.

Various constituents of electrode coating are cellulose, calcium fluoride, calcium carbonate, titanium dioxide, clay, talc, iron oxide, asbestos, potassium / sodium silicate, iron powder, ferro-maganese, powdered alloys, silica etc. Each constituent performs either one or more than one functions.

Electrode metallic core wire is the same but the coating constituents give the different characteristics to the welds. Based on the coating constituents, structural steel electrodes can be classified in the following classes;

  1. Cellulosic Electrodes

    Coating consists of high cellulosic content more than 30% and TiO2 up to 20%. These are all position electrodes and produce deep penetration because of extra heat generated during burning of cellulosic materials. However, high spatter losses are associated with these electrodes.

  2. Rutile Electrodes

    Coating consists of TiO 2 up to 45% and SiO2 around 20%. These electrodes are widely used for general work and are called general purpose electrodes.

  3. Acidic Electrodes

    Coating consists of iron oxide more than 20%. Sometimes it may be up to 40%, other constituents may be TiO2 10% and CaCO3 10%. Such electrodes produce self detaching slag and smooth weld finish and are used normally in flat position.

  4. Basic Electrodes

    Coating consist of CaCO3 around 40% and CaF2 15-20%. These electrodes normally require baking at temperature of approximately 250 ° C for 1-2 hrs or as per manufacturer's instructions. Such electrodes produce high quality weld deposits which has high resistance to cracking. This is because hydrogen is removed from weld metal by the action of fluorine i.e. forming HF acid as CaF2 generates fluorine on dissociation in the heat of arc.

 Table 5.3: Coating Constituents and Their Functions

Coating Constituent

Functions

Main Functions

Other Functions

Cellulose

Gas former

Coating Strength and Reducing agent

Calcium Fluoride (CaF2)

Slag basicity and metal fluidity, H2 removal

Slag former

Clay (Aluminum Silicate)

Slag former

Coating strength

Talc (Magnesium Silicate)

Slag former

Arc stabilizer

Rutile (TiO2 )

Arc stabilizer, Slag former, Fluidity

Slag removal and bead appearance

Iron Oxides

Fluidity, Slag former

Arc Stabilizer, improved metal transfer,

Calcium Carbonate

Gas former, Arc stabilizer

Slag basicity, Slag former

Asbestos

Coating strength

Slag former

Quartz (SiO2 )

Slag fluidity, Slag former

Increase in current carrying capacity.

Sodium Silicate / Potassium Silicate

Binder, Arc stabilizer

Slag former

FeMn / FeSi

Deoxidizer

-

Iron Powder

Deposition Rate

-

Powdered Alloys

Alloying

-

 

Classification of Electrodes as per Indian Standard:

Structural steel electrodes were classified as per IS 814:1974 and this code was revised and the revised code is IS 814:1991.

The corresponding code is given on each packet of electrode.

IS 815:1974

As per IS 815 electrodes are designated with letters and digits.

P X X X X X X S

Prefix (P) is either E or R which indicates solid extruded (E) or reinforced extruded (R) Electrode.

1 st digit – Indicates type of coating.

2 nd digit – Indicates weld positions in which electrode can be used.

3 rd digit – Indicates welding current conditions.

4 th and 5 th digit – Indicate UTS and YS of all weld metal.

6 th digit – Requirement of minimum % elongation and absorbed energy in charpy V- notch impact test of weld metal.

Suffix (s) – P – Deep penetration electrode

H – Hydrogen controlled electrode

J, K and L – Amount of metal recovery in case of iron powder electrode

Suffix (s) are optional and may or may not be given if not applicable.

IS 814:1991

As per IS 814 electrodes are designated with letters and digits as given below:

E L X X X X S

In this code E indicates extruded solid electrode, L is a letter to designate type of coating, first digit indicates UTS and YS of deposited weld metal, second digit gives percentage elongation and impact values of weld metal deposited, third digit gives welding positions in which electrode can be used and fourth digit gives the current conditions for the use of electrode.

Suffix(s) are optional and indicate special characteristics of electrode such as H1, H2, and H3 indicate hydrogen controlled electrodes with different amount of diffusible hydrogen J, K, L indicate different amount of metal recovery in weld pool in case of iron powder electrodes and X means radiographic weld quality.  

Note: For details see the above codes published by Bureau of Indian Standards (BIS), Manak Bhawan, Bahadur Shah Jafar Marg, New Delhi .

Weld Bead Geometry

Figure 5.3 shows the important parameters of the weld bead geometry for a butt weld.

FIg 5.3: Weld Bead Geometry